Hi all,
I was after some advice regarding qld maple. Our LMI bender arrived yesterday, after we unpacked it, shook our heads at the price again, we got into some qld sides. But they are cracking. As we are at a loss, I thought that would seek out your collective wisdom. We have it set at 350 for the waist and 300 for the bouts. We lightly sprayed with water before bending. All as per instructions. Any advice is greatly appreciated. Thanks in advance,
Daniel.

User avatar
kiwigeo
Admin
Posts: 10687
Joined: Sat Sep 29, 2007 5:57 pm
Location: Adelaide, Sth Australia

Re: Queensland Maple bending problems

Post by kiwigeo » Sat Jul 30, 2011 11:40 am

You're using bending slats etc? What's the stack sequence with bending slats, wood, blanket etc?
Martin

User avatar
Daniel_M
Blackwood
Posts: 122
Joined: Mon Jan 31, 2011 5:15 pm
Location: North Parramatta

Re: Queensland Maple bending problems

Post by Daniel_M » Sat Jul 30, 2011 1:05 pm

Hi Martin,
Sure am. Small bending slat for waist, large bending slat, large heat blanket,wood, small heat blanket for waist, large bending slat. There is two heat readers in there a well - just small wires. This is per the instructions. The procedure is let it get to 350 then quarter turn every 30 seconds. Which is not very much at all. Do you think soaking the wood would help? Would this be a sign that the wood was not perfectly quartered?

Thanks again,
Daniel.

jeffhigh
Blackwood
Posts: 1536
Joined: Thu Feb 07, 2008 5:50 am
Location: Caves Beach, NSW
Contact:

Re: Queensland Maple bending problems

Post by jeffhigh » Sat Jul 30, 2011 1:11 pm

Perhaps runout in the wood rather than off quarter.
I have only bent Qld maple by hand on a bending iron but found it one of the easier woods to bend.

User avatar
Bob Connor
Admin
Posts: 3126
Joined: Mon Jul 09, 2007 9:43 pm
Location: Geelong, Australia
Contact:

Re: Queensland Maple bending problems

Post by Bob Connor » Sat Jul 30, 2011 7:47 pm

How thick are the sides?
Bob, Geelong
_______________________________________

Mainwaring and Connor Guitars

User avatar
Daniel_M
Blackwood
Posts: 122
Joined: Mon Jan 31, 2011 5:15 pm
Location: North Parramatta

Re: Queensland Maple bending problems

Post by Daniel_M » Sat Jul 30, 2011 8:30 pm

Hey Bob,
I took them down to 2.5mm. There is a possibility that they may not have been dry enough - I need to get a new moisture meter.

Thanks,
Dan.

User avatar
Bob Connor
Admin
Posts: 3126
Joined: Mon Jul 09, 2007 9:43 pm
Location: Geelong, Australia
Contact:

Re: Queensland Maple bending problems

Post by Bob Connor » Sat Jul 30, 2011 8:59 pm

I used to take sides down to .080-.085" (2-2.1mm) when I was building with single ply sides.

I reckon they're a little thick. Moisture in them shouldn't make them crack when bending. Quite the opposite really.

I now build with laminated sides with each (of two) laminates being .045" (1.2mm or thereabouts)

Regards
Bob, Geelong
_______________________________________

Mainwaring and Connor Guitars

User avatar
Daniel_M
Blackwood
Posts: 122
Joined: Mon Jan 31, 2011 5:15 pm
Location: North Parramatta

Re: Queensland Maple bending problems

Post by Daniel_M » Sat Jul 30, 2011 10:03 pm

Thanks again Bob. I am about to build a double side sheoak OM so that info is handy! Will try with those at 1.2mm. :)

Pete Brown
Blackwood
Posts: 115
Joined: Tue Dec 09, 2008 1:15 pm

Re: Queensland Maple bending problems

Post by Pete Brown » Sun Jul 31, 2011 3:15 am

Daniel_M wrote:We have it set at 350 for the waist and 300 for the bouts.
Daniel, I can't speak authoritatively as I haven't built with Queensland maple, but I"d suggest that by allowing the wood to reach 350 before beginning the bend, the wood may well have dried out completely before the bends are completed, thus contributing to the cracking you've experienced. Common wisdom has it that bending should begin at the waist when the temperature is at around 240F. For the majority of wood species, the maximum recommended temperature is around 300F.

For guidance from someone far more experienced than I am, John Mayes outlines his side bending process and recommended temperatures part way down this page:
http://www.lint.org/TechNotes/Mayes/MayesNotes.html

Cheers
Pete

User avatar
xray
Blackwood
Posts: 148
Joined: Sun Aug 24, 2008 5:01 pm

Re: Queensland Maple bending problems

Post by xray » Sun Jul 31, 2011 4:20 pm

hi daniel, i have bent stacks of maple and as a rule of thumb soaking the stuff doesn't hurt. I usually find that the maple i have is not very thirsty initially and dries out fast under a heat blanket. Bend the waist first and stop to let it cool down. Take it out of your bender and re wet to be sure it is not too dry. You dont have to soak it at this stage just enough to wet the surface.
hope this helps.

User avatar
kiwigeo
Admin
Posts: 10687
Joined: Sat Sep 29, 2007 5:57 pm
Location: Adelaide, Sth Australia

Re: Queensland Maple bending problems

Post by kiwigeo » Sun Jul 31, 2011 8:30 pm

I wrap my sides in al foil after spritzing them with a bit of water.....slows down the loss of water as steam.
Martin

User avatar
Daniel_M
Blackwood
Posts: 122
Joined: Mon Jan 31, 2011 5:15 pm
Location: North Parramatta

Re: Queensland Maple bending problems

Post by Daniel_M » Sun Jul 31, 2011 11:02 pm

Thanks all for all the great help and suggestions.
I am trying again next weekend, but after all the advice it seems like we had the heat blankets too hot and this was drying out the timber. As per advice I will be re spraying half way and also making seal with the tinfoil better - I just had it folded over and not really sealed. Thanks again gents. :cl :cl :D

User avatar
graham mcdonald
Blackwood
Posts: 473
Joined: Thu Oct 25, 2007 11:57 am
Location: Canberra
Contact:

Re: Queensland Maple bending problems

Post by graham mcdonald » Mon Aug 01, 2011 8:30 am

Sides should be around 2mm /.080" thick. There is no need for them to be any thicker. Spray with water, wrap in paper towel (one layer each side), spray again, wrap in aluminium foil, as sealed as possible and mark with something so you know which side/edge is which so you can maintain the bookmatching. Place the wrapped package between slats - aluminium, stainless or whatever - and bend. When the temp gets up towards 300F they should just go like cardboard and you can pull them into shape with little effort. Getting the foil as sealed as possible keeps the steam in and they should bend with no problems. Qld maple is pretty good bending timber.

cheers

graham
Graham McDonald
http://www.mcdonaldstrings.com

Drommy
Gidgee
Posts: 6
Joined: Thu Jul 16, 2009 11:37 am
Location: Mackay

Re: Queensland Maple bending problems

Post by Drommy » Thu Aug 04, 2011 9:39 am

Hi,Daneil.
In the past i've soaked maple in warm water before bending and this has worked fine adding a spray of water as i bend. good luck.

User avatar
Daniel_M
Blackwood
Posts: 122
Joined: Mon Jan 31, 2011 5:15 pm
Location: North Parramatta

Re: Queensland Maple bending problems

Post by Daniel_M » Thu Aug 04, 2011 10:36 am

thanks gents,

I am bending on the weekend again so will no doubt post of my success (finger's crossed!) :wink:


Daniel

Bruce McC
Blackwood
Posts: 396
Joined: Thu Apr 07, 2011 1:29 pm
Location: Canberra ACT Australia

Re: Queensland Maple bending problems

Post by Bruce McC » Thu Aug 04, 2011 10:58 am

Hi Daniel
I have just finished bending mahogany sides in a "Fox" type bender. As a heat source I use 3 halogen bar lamps (2 x 200W + 1 x 150W)
and use two stainless steel slats approx 0.6 mm. I prepared my sides as described by Graham McD above and the sides bent easily with out any issues.
Hope it all goes well for you on the week end.